Low-alloy steels Manual éléktroda E8016-B2 logam Jointing barang
éléktroda leungeun tipe kalium hidrogén low, busur stabil, kirang Santika, molding alus, panyabutan slag gampang
Kinerja X-Ray alus teuing
Sipat mékanis stabil, kateguhan dampak anu luhur tiasa dijaga dina kaayaan perlakuan panas
KOMPONEN KIMIA:
PADUNGAN (wt%) | C | Si | Mn | P | S | Ni | Cr | Mo | Lain |
ATURAN GB/T | 0.081 | 0.32 | 0.72 | 0.017 | 0.011 | 0.013 | 1.2 | 0.5 | - |
SIFAT MEKANIKAL:
HARTA | Kakuatan ngahasilkeun (MPa) | Kakuatan éksténsif (MPa) | Elongation(%) | NILAI IMPAK J/℃ | Perlakuan panas °C*h | |||||
ATURAN GB/T | 480 | 580 | 22 | 150/suhu normal | 690*1 |
Parameter las anu disarankeun:
SPESIFIKASI DIAMETER (mm) | 3.2*350 | 4.0*400 | 5.0*400 | ||||
LISTRIK (Amp) | H/W | 90-130 | 140-190 | 190-240 | |||
O/W | 80-120 | 120-160 | - |
-
20,00 TEU kapal kontainer
-
Proyék YAMAL LNG
-
Sanmen 2 # teu aktip
KOMPONEN KIMIA:
PADUNGAN (wt%) | C | Si | Mn | P | S | Ni | Cr | Mo | Lain |
ATURAN GB/T | 0.081 | 0.32 | 0.72 | 0.017 | 0.011 | 0.013 | 1.2 | 0.5 | - |
SIFAT MEKANIKAL:
HARTA | Kakuatan ngahasilkeun (MPa) | Kakuatan éksténsif (MPa) | Elongation(%) | NILAI IMPAK J/℃ | Perlakuan panas °C*h | |||||
ATURAN GB/T | 480 | 580 | 22 | 150/suhu normal | 690*1 |
Parameter las anu disarankeun:
SPESIFIKASI DIAMETER (mm) | 3.2*350 | 4.0*400 | 5.0*400 | ||||
LISTRIK (Amp) | H/W | 90-130 | 140-190 | 190-240 | |||
O/W | 80-120 | 120-160 | - |
Tulis pesen anjeun di dieu sareng kirimkeun ka kami