Low-alloy steels Manual éléktroda E8018-C2 data Soldering
KOMPONEN KIMIA:
PADUNGAN (wt%) | C | Mn | Si | Ni | Cr | Mo | P | S |
ATURAN GB/T | 0.12 | 1.25 | 0.80 | 3.00-3.75 | - | - | 0.03 | 0.03 |
ATURAN AWS | 0.12 | 1.25 | 0.80 | 3.00-3.75 | - | - | 0.03 | 0.03 |
NILAI CONTOH | 0.045 | 0.75 | 0.22 | 3.52 | 0.04 | 0.06 | 0.007 | 0.004 |
PILIHAN MEKANIKAL:
HARTA | Kakuatan ngahasilkeun (MPa) | Kakuatan éksténsif (MPa) | NILAI IMPAK J/℃ | ELONGATION(%) | perlakuan panas °Cxh | |||||
ATURAN GB/T | 460 | 550 | 27/-75 | 17 | 605*1 | |||||
ATURAN AWS | 460 | 550 | 27/-75 | 19 | 605*1 | |||||
NILAI CONTOH | 495 | 600 | 100/-75 | 26 | 605*1 |
Parameter las anu disarankeun:
SPESIFIKASI DIAMETER (mm) | 2.6*350 | 3.2*350 | 4.0*400 | 5.0*400 | ||||
LISTRIK (Amp) | H/W | 80-110 | 100-130 | 130-180 | 170-210 | |||
O/W | 60-100 | 80-120 | 120-160 | - |
Beusi bubuk éléktroda leungeun tipe hidrogén low.
Kusabab ditambah bubuk beusi, efisiensi lebur leuwih luhur, dampak kateguhan logam molten dina -75 ℃.
arc stabil, kirang Santika, ngabentuk alus, panyabutan slag gampang, kinerja X-Ray téh alus teuing.
KOMPONEN KIMIA:
PADUNGAN (wt%) | C | Mn | Si | Ni | Cr | Mo | P | S |
ATURAN GB/T | 0.12 | 1.25 | 0.80 | 3.00-3.75 | - | - | 0.03 | 0.03 |
ATURAN AWS | 0.12 | 1.25 | 0.80 | 3.00-3.75 | - | - | 0.03 | 0.03 |
NILAI CONTOH | 0.045 | 0.75 | 0.22 | 3.52 | 0.04 | 0.06 | 0.007 | 0.004 |
PILIHAN MEKANIKAL:
HARTA | Kakuatan ngahasilkeun (MPa) | Kakuatan éksténsif (MPa) | NILAI IMPAK J/℃ | ELONGATION(%) | perlakuan panas °Cxh | |||||
ATURAN GB/T | 460 | 550 | 27/-75 | 17 | 605*1 | |||||
ATURAN AWS | 460 | 550 | 27/-75 | 19 | 605*1 | |||||
NILAI CONTOH | 495 | 600 | 100/-75 | 26 | 605*1 |
Parameter las anu disarankeun:
SPESIFIKASI DIAMETER (mm) | 2.6*350 | 3.2*350 | 4.0*400 | 5.0*400 | ||||
LISTRIK (Amp) | H/W | 80-110 | 100-130 | 130-180 | 170-210 | |||
O/W | 60-100 | 80-120 | 120-160 | - |
Tulis pesen anjeun di dieu sareng kirimkeun ka kami